Time: 2019-12-12

1) Preparation of MEKO-end-capped PU prepolymer solution

Formulation:

  Parts(w/w)
a. α,α,α',α'-Tetramethyl Xylylene Diisocyanate 259
b. Carbitol Acetate 400
c. Trimethylolpropane 28
d. Polybutanol 212
e. Dibutyltin Dilaurate 0.1
f. MEKO 101

Add ingredients a,b, c,d and e into a reactor fitted with a stirrer, heater, thermometer and gas inlet. Heat to 80~100 while stirring under nitrogen and keep for 3hr to allow max. PU prepolymer yield, that is NCO% reaches 8.9%. Add MEKO (ingredient f) into the solution and react at 60~80 for 3hr until NCO peaks disappear by IR detection. Thus MEKO end-capped PU prepolymer solution, with 60% of solid content, is obtained.

2) Preparation of the coating

Formulation:

g. MEKO end-capped PU prepolymer solution 100
h. Carbon Black 1
i. Titanium Dioxide 5
j. Calcium Carbonate 80
k. Aromatic Naphtha (bp. 100~200) 30

Place the above ingredients in a mixer, and mix thoroughly to achieve a uniform suspension.

Characteristics and Use:

1. High adhesion, impact resistance and storage stability.

2. Suitable for galvanized steel surface, automotive, etc.

3. Recommended to apply by air spray; bake at 120 for 15min; film thickness 20μm. It can also be applied by brush, roller, blade and E-coating.

Support hotline:

+86-570-3687898

Tech. Support: +86-13906706367

Fax: +86-570-3375533

E-mail: kailin1133@kailinchem.com

Website: www.kailinchem.com

Copyright(C)2019, Zhejiang Sainon Chemical Co., Ltd. All Rights Reserved. Supported by ChemNet ChinaChemNet Toocle Copyright Notice